化學配方數(shù)據(jù)庫
配方類型: POLISH
配方說明: Liquid Solvent Floor Polish
配方組成: Stoddard Solvent/89
"Petrolite" P-25
Paraffin Wax, 140 AMP/7-6
"Petrolite" P-20/4-6
Formula No.
"Petrolite" P020
"Petrolite" P-25/4-5
Paraffin Wax, 140 AMP/7-6
Stoddard Solvent/89
配制方法: Heat solvent to 180F and add molten waxes. Cool with stirring and pour into containers between 100F and 140F.
Caution: do not stir rapidly when mixture approaches pouring temperatures. Rapid agitation will adversely affect the formation of crystals and may cause separation of solvent.
P-20 and P-25 have excellent solvent-binding properties and if the polish is compounded properly, there should be less than 5% of free solvent. P-20 and P-25 have very similar properties, but P-25 is recommended when a viscous gel is desired.
The formulas given contain 11% solids and have a good cleaning action during application. The finished wax film is free from tack and buffs readily to a high gloss. The hardness of the film can be regulated by varying the ratio of synthetic wax to paraffin.